Precipitation-Hardening Stainless Steel · Airframe-Grade Bolting

PH13-8Mo Stainless Steel Fasteners

UNS S13800 EN / DIN 1.4534 AMS 5629 AMS 5864 ASTM A564

Jiangsu Calverbolt Fasteners Co., Ltd. manufactures and exports PH13-8Mo (13-8 Mo, UNS S13800, EN/DIN 1.4534) precipitation-hardening stainless steel fasteners — hex bolts, heavy hex bolts, stud bolts, threaded rod, socket head cap screws, nuts and washers, plus fully made-to-drawing parts — machined from vacuum-melted, airframe-quality bar and supplied in every standard aging condition from H950 to H1150.

1517 MPaMax UTS · H950 · 220 ksi min
H950–H1150Aging conditions
1/4"–4"Diameter range
3.1 certEN 10204 on request
UNS S13800 · 1.4534 PH13-8Mo stainless steel stud bolts and heavy hex nuts securing a high-pressure pipeline flange
PH13-8Mo stud bolts & heavy hex nuts on a high-pressure flanged joint.

What Is PH13-8Mo Stainless Steel?

A direct answer for specifiers: the chemistry, the mechanism and why 13-8Mo bolts exist.

PH13-8Mo — also written 13-8Mo or PH 13-8 Mo, UNS S13800, EN/DIN 1.4534 — is a martensitic precipitation-hardening (maraging) stainless steel that combines very high strength and hardness with superior fracture toughness and good resistance to general corrosion and stress-corrosion cracking (SCC).

Strength comes from a single low-temperature age-hardening treatment: after solution treating, aging precipitates an aluminium-rich NiAl phase inside a chromium-nickel-molybdenum martensitic matrix. Tight composition control, a low carbon content (0.05% max) and vacuum or double-vacuum melting keep impurities and segregation minimal — which is where the grade's signature excellent transverse toughness and minimal directionality come from. For a bolt loaded across its section, that means predictable performance in every direction, not just along the bar.

The alloy is magnetic in every condition, age-hardens through a single low-temperature treatment, and has become the standard choice wherever 17-4PH-class strength must survive sustained load in a corrosive or marine atmosphere — see the corrosion data.

PH13-8Mo: Every Name, Number & Specification in One Place

Buyers and engineers search this grade under many names. This is the full cross-reference, so your RFQ matches whatever your drawing, ERP or standard calls out.

Designations and equivalents for PH13-8Mo stainless steel
DesignationSystemNotes
PH13-8Mo / 13-8MoTrade / commonThe most common industry spellings; "13-8" from the nominal 13% Cr – 8% Ni chemistry
PH 13-8 MoTrademark"PH 13-8 Mo" is a registered trademark historically associated with Armco Inc.
UNS S13800UNS (USA)Unified Numbering System designation
1.4534EN / DIN (Europe)Material number used on EN and DIN documentation
Specifications covering PH13-8Mo fastener stock
SpecificationCoversRole for fasteners
AMS 5629Bars, forgings & ringsBolting stock for bolts, studs, nuts and machined parts
AMS 5864Sheet, strip & plateShims, brackets, gasket-faced parts; source of the minimum-property tables
ASTM A564 / A564MBars, wire & forgingsCommercial and industrial bolting stock

Ordering tip: put the melting route (vacuum melted for airframe work), the aging condition (e.g. H1000) and the certification level (EN 10204 3.1) on the same line as the fastener description — we quote exactly to that line.

PH13-8Mo Fastener Product Range

Every product below is manufactured in-house by cold heading and precision machining, in diameters from 1/4" to 4" (metric equivalents on request), to ANSI/ASME, ASTM, DIN, ISO, BS or GB dimensions — or to your drawing.

01 / BOLTS

PH13-8Mo Hex Bolts

Hex head cap bolts, partially or fully threaded, in UNC, UNF and metric threads, from 1/4" through 4" diameter and in every aging condition.

02 / BOLTS

13-8Mo Heavy Hex Bolts

Heavy hex bolting for structural and pressure-boundary joints where a larger bearing surface and high preload are required.

03 / STUDS

PH13-8Mo Stud Bolts & Threaded Rod

Double-end studs, tap-end studs, full-thread and partial-thread stud bolts and threaded rod for flanged and turbine joints.

04 / SCREWS

13-8Mo Socket Head Cap Screws

Hex socket head cap screws, flat and button head screws, machined or cold-headed with precision-rolled threads.

05 / NUTS

PH13-8Mo Nuts

Hex nuts, heavy hex nuts, jam nuts and flange nuts in matched PH13-8Mo chemistry and condition for the bolted system.

06 / WASHERS

13-8Mo Washers & Pins

Flat washers, lock washers, precision pins and dowel components produced to tight geometric tolerance.

07 / CUSTOM

Made-to-Drawing Fasteners

Non-standard bolts, special studs, shafts and cold-formed parts machined from PH13-8Mo bar to your drawing and inspection plan.

The Condition Ladder: Strength vs. Aging Temperature

PH13-8Mo is ordered by aging condition. The lower the aging temperature, the higher the strength; the higher the aging temperature, the higher the toughness and SCC margin. Every bar below is a certified minimum you can order to.

  • H950 — maximum strength and hardness (220 ksi UTS, 45 HRC min) for pins, screws and highly loaded studs in compact sections.
  • H1000 — the engineering optimum for structural bolting: 205 ksi UTS with the highest SCC margin among high-strength conditions.
  • H1025 / H1050 — strength-toughness steps used where ductility and fracture toughness carry more weight than peak strength.
  • H1100 / H1150 — maximum toughness and dimensional stability for large sections, weldments and machinability-critical parts.
  • RH950 — subzero-treated route that raises strength at H950 level in heavier sections; specified in some airframe standards.
  • H1150M — double-aged, overaged condition giving optimum machinability; parts are then re-solution treated and re-aged to final properties.

Not sure which condition to order? Send us the load case and service environment — our engineers will recommend the condition, thread class and finish, and quote to them.

Ask an Engineer

Chemical Composition — UNS S13800 / 1.4534

Tight limits, low impurities: the reason PH13-8Mo fasteners are tough in every direction.

Chemical composition limits of PH13-8Mo stainless steel, UNS S13800, EN 1.4534, percent by weight
ElementMin (%)Max (%)Why it matters
Chromium (Cr)12.2513.25Corrosion resistance, martensitic hardenability
Nickel (Ni)7.508.50Toughness, austenite balance
Molybdenum (Mo)2.002.50Corrosion resistance, temper resistance
Aluminium (Al)0.901.35Forms NiAl precipitates — the age-hardening phase
Carbon (C)—0.05Kept low for weldability and toughness
Manganese (Mn)—0.10Impurity control
Silicon (Si)—0.10Impurity control
Phosphorus (P)—0.010Impurity control
Sulfur (S)—0.008Impurity control — cleanliness for transverse ductility
Nitrogen (N)—0.01Controlled to keep aging response predictable
Iron (Fe)balance—

Source limits: AMS 5629 / AMS 5864 chemistry for UNS S13800. Vacuum melting (VIM/VAR) applies for airframe-quality lots.

Mechanical Properties by Aging Condition

Minimum room-temperature properties Calverbolt certifies PH13-8Mo fastener stock to, per AMS 5864.

Minimum mechanical properties of PH13-8Mo UNS S13800 by aging condition per AMS 5864
ConditionUTS ksi (MPa)0.2% YS ksi (MPa)Elong. in 2" %RA % minHardness HRC min
H950220 (1517)205 (1413)104545
H1000205 (1413)190 (1310)105043
H1025185 (1276)175 (1207)1150—
H1050175 (1207)165 (1138)125040
H1100150 (1034)135 (931)145034
H1150135 (931)90 (621)145030

UTS = ultimate tensile strength; YS = 0.2% offset yield strength; RA = reduction of area. Transverse and short-transverse minimums per AMS 5864 apply; ask for the full test certificate.

Physical Properties

Physical properties of PH13-8Mo stainless steel
Density (H1000)7.76 g/cm³ · 0.280 lb/in³ · 7760 kg/m³
Melting range2560–2680 °F · 1404–1471 °C
Modulus of elasticity (RT)29.0 × 10⁶ psi · ≈200 GPa
Electrical resistivity (Condition A, 100 °C)613 Ω·circ-mil/ft · ≈1020 µΩ·cm
Thermal conductivity (Condition A, 100 °C)14.0 W/m·K · 97.2 Btu·in/(ft²·h·°F)
Thermal expansion, 21–482 °C (H950)11.9 × 10⁻⁶/K
Magnetic permeability (H950)≈46–127 at 10.5–264 Oe
Size change on aging (H1000)0.0004–0.0006 in/in contraction
  • Ferromagnetic in all conditions — unlike austenitic 304/316 bolts, PH13-8Mo bolting responds to magnetic inspection methods.
  • Low thermal expansion — close to ferritic steels; useful where bolted joints cycle with temperature.
  • Predictable size change on aging — machinists can compensate for the 0.04–0.06% contraction before final aging.
  • Oxidation resistance to about 1100 °F (593 °C) in service; short excursions kept at least 50 °F below the aging temperature.

PH13-8Mo vs 17-4PH, 15-5PH, A286, Inconel 718 & 316

Where the grade sits against the alternatives buyers most often cross-quote — minimum properties per the referenced specification, each at its standard bolting condition.

Comparison of PH13-8Mo with 17-4PH, 15-5PH, A286, Inconel 718 and 316 stainless steel minimum mechanical properties
Grade (condition)UNSSpecUTS min, ksi (MPa)YS min, ksi (MPa)Key difference vs PH13-8Mo
PH13-8Mo (H950)S13800AMS 5864*220 (1517)205 (1413)Highest strength with the best transverse toughness of the PH stainless family
PH13-8Mo (H1000)S13800AMS 5864*205 (1413)190 (1310)Best SCC margin at high strength — the airframe workhorse
17-4PH (H900)S17400AMS 5643190 (1310)170 (1170)Economical and widely stocked; less transverse toughness, more directionality
15-5PH (H900)S15500AMS 5659190 (1310)170 (1170)Similar class to 17-4 with better through-section property uniformity
A286 (aged)S66286AMS 5737140 (965)95 (655)Iron-nickel superalloy for sustained service to about 1000 °F; lower strength
Inconel 718 (aged)N07718AMS 5662185 (1275)150 (1034)Nickel superalloy for service to about 1200 °F and sour gas; higher cost
316 (annealed)S31600ASTM A27675 (515)30 (205)Austenitic, non-magnetic, top general corrosion resistance; far lower strength

*PH13-8Mo minimums shown per AMS 5864; bar-stock lots are certified to the ordered specification and condition. Comparison minimums: 17-4PH per AMS 5643, 15-5PH per AMS 5659, A286 per AMS 5737, 718 per AMS 5662, 316 per ASTM A276 annealed. INCONEL is a trademark of Special Metals Corporation.

How to choose, in one line each: maximum strength plus maximum toughness → PH13-8Mo H950/H1000; general corrosion at modest strength → 316; economy at the 190-ksi class → 17-4PH or 15-5PH; sustained temperature above roughly 800–900 °F → A286 or Inconel 718. Send us the load case and environment if the choice is not obvious — we size the grade and condition for you.

How We Make a PH13-8Mo Bolt

Every step is a controlled process — and each one is traceable on your EN 10204 3.1 certificate.

  1. Vacuum-melted bar stock

    Airframe-quality PH13-8Mo produced by vacuum or double-vacuum melting (VIM/VAR) to AMS 5629 — the clean melt that delivers transverse toughness in the finished fastener.

  2. Solution treat — Condition A

    Heat at 1675–1725 °F (910–940 °C) for 15–30 minutes per section, then cool below 60 °F (15 °C) to transform the structure fully to martensite.

  3. Head, thread & machine

    Cold heading, thread rolling and machining are carried out in Condition A. Sections previously overaged to H1150M for machinability are re-solution treated before final aging.

  4. Age harden

    Hold at the ordered condition temperature 950–1150 °F (510–621 °C) ± 10 °F for 4 hours, air cool. RH950 adds a −100 °F subzero treatment within 24 h of solution treating; H1150M is a 1400 °F + 1150 °F double age.

  5. Test & passivate

    Tensile, hardness and proof testing per the ordered standard, thread gauging, then pickling and passivation — finished parts must be free of scale and heat tint for full corrosion performance.

Welding, Cutting & Re-Machining PH13-8Mo Hardware

The fabrication rules that protect the properties you are paying for.

  • Welding: best performed in the solution-treated condition, followed by re-solution treating and aging. Welded-and-re-aged joints retained a high level of stress-corrosion-cracking resistance in marine atmospheric testing.
  • Brazing: heat treatment may be done in inert atmospheres — reducing atmospheres must not be used, because of the potential for nitrogen contamination.
  • Overaged parts: H1150 and H1150M material will not respond to further aging — re-solution treat at 1700 °F after forging or heavy machining, before final aging to the ordered condition.
  • Cutting: saw or cold-cut bar and billets; abrasive-wheel cutting of annealed stock can introduce fine surface cracks and should be avoided.
  • Machining: good tool life in Condition A at speeds about 20–30% below 304-type practice; H1150M provides optimum machinability and is the route we use for complex made-to-drawing parts before re-solution treating and re-aging.

Corrosion & Stress-Corrosion-Cracking Resistance

Why specifiers replace 17-4PH and B8 bolts with PH13-8Mo in aggressive atmospheres.

In the H950 condition, PH13-8Mo shows rusting resistance similar to Type 304 stainless in a 5% salt-fog test, and in atmospheric exposure its general-corrosion resistance likewise approaches Type 304.

The grade's decisive advantage is stress-corrosion-cracking resistance. In long-term marine atmospheric testing on smooth bent-beam specimens, H1000 and H1050 material loaded to 75–100% of its yield strength showed no failure in 1,405 days of exposure; welded-and-reaged material performed identically.

For the best SCC margin, order H1000 or above — a minimum aging temperature of 1000 °F (538 °C) is recommended. Long-term service between roughly 600–900 °F (315–480 °C) can reduce toughness in PH grades; our engineers flag this and propose a higher aging condition where needed.

Temperature Capability & Service-Environment Limits

The temperature limits for PH13-8Mo bolting, stated the way a specifier needs them.

  • Oxidation resistance to about 1100 °F (593 °C) — the alloy's demonstrated limit in air service.
  • Watch 600–900 °F (315–480 °C): long-term exposure in this band can reduce toughness in precipitation-hardening stainless steels; using a higher aging condition (H1100 / H1150) minimises the effect.
  • Short excursions: acceptable with the metal temperature kept at least 50 °F (28 °C) below the fastener's aging temperature.
  • Marine atmospheres: smooth specimens in H1000/H1050 carried 75–100% of yield strength for 1,405 days without stress-corrosion cracking.
  • Cryogenic or sub-zero certificates: send the test temperature and acceptance criteria — we quote lot-tested hardware to match.

Where PH13-8Mo Fasteners Are Specified

AEROSPACE

Airframe Structural Bolting

Highly loaded structural joints where strength and fracture toughness must both be certified — 13-8Mo's transverse toughness is the reason airframe designers choose it.

AEROSPACE

Landing Gear & Actuation

Landing-gear pins, links, clevises and actuator bolts in H1000, where shock loading and corrosion resistance combine.

OIL & GAS

Valves, Fittings & Wellhead Bolting

Valve trim fasteners, fittings, studs and pressure-boundary bolting exposed to sour or marine atmospheres.

PETROCHEMICAL

High-Pressure Flanged Joints

Stud bolts and nuts for petrochemical equipment where sustained high preload must not relax in a corrosive environment.

POWER / NUCLEAR

Nuclear Reactor Components

Bolting for nuclear reactor internals and support structures, specified for its combination of strength and SCC resistance.

TOOLING

Injection Molding Equipment

Tie-bars, clamping and manifold bolting in molding machines — high strength under cyclic load and humidity.

Quality, Testing & Certification

  • EN 10204 type 3.1 material test certificates with every certified lot — actual chemistry and mechanical results, not typical values.
  • Full lot traceability from melt route to finished fastener, with heat numbers on all shipping documents.
  • Tensile, yield, hardness and proof-load testing to the ordered fastener standard; elongation and reduction of area recorded.
  • PMI / OES chemistry verification of incoming PH13-8Mo bar stock before production release.
  • NDT on request — dye-penetrant and eddy-current inspection for critical hardware.
  • Thread gauging and dimensional inspection to ANSI/ASME, DIN, ISO, BS, GB or your drawing, with inspection reports supplied.
  • Passivation and pickling after heat treatment for the maximum corrosion performance the grade can deliver.
Precision-rolled threads on PH13-8Mo UNS S13800 high-strength stainless steel hex bolts
Precision-rolled threads on PH13-8Mo hex bolts — rolled threads add fatigue strength over cut threads.

Why Source PH13-8Mo Fasteners from Calverbolt

01

One Grade in a Master Library

PH13-8Mo is one of 800+ material grades we run — duplex, super duplex, Inconel 718, Monel, Hastelloy, A286 and more — so mixed-material orders ship together, from one plant, under one certificate.

02

Complete Range, Flexible Quantities

1/4" through 4" diameter, standard and non-standard, bolts, studs, nuts, washers and made-to-drawing parts — sampled, short-run or production quantities.

03

Engineering-Led Quoting

Send a standard, a grade or a drawing. Our engineers match material, dimensions and finish to your service conditions — high temperature, cryogenic, seawater, sour service or heavy load.

04

All Dimensional Systems

GB, DIN, ANSI, ASME, ASTM, ISO and BS threading and dimensional standards from stock tooling, or fully custom geometry.

05

Export-Ready Documentation

EN 10204 3.1 certificates, inspection reports, seaworthy export packing and full shipping documentation from Dongtai, Jiangsu.

06

Direct From the Manufacturer

Factory pricing and lead times, no trading layer — WhatsApp and email answered by the sales engineers who run the order.

PH13-8Mo Rod Weight Table — for Shipping & Costing

Theoretical weight of plain PH13-8Mo rod at 7.76 g/cm³ — the number freight quotes and material-cost estimates start from. Finished bolts and studs weigh less once threads are rolled.

Theoretical weight per metre and per foot of PH13-8Mo round rod by diameter
Rod diameterkg/mlb/ftCommon fastener use
1/4" (6.35 mm)0.250.17Screws, pins, small studs
3/8" (9.53 mm)0.550.37Screws, small bolts
1/2" (12.7 mm)0.980.66Standard flange bolting
5/8" (15.88 mm)1.541.03Studs, hex bolts
3/4" (19.05 mm)2.211.49Structural & valve bolting
1" (25.4 mm)3.932.64Heavy studs, airframe joints
1-1/4" (31.75 mm)6.144.13Large studs, pins
1-1/2" (38.1 mm)8.855.95Heavy flange studs
2" (50.8 mm)15.7310.57Pressure-boundary studs
2-1/2" (63.5 mm)24.5816.52Large machined parts
3" (76.2 mm)35.3923.78Billet, custom forgings
4" (101.6 mm)62.9242.28Billet, made-to-drawing parts

kg/m = 0.006095 × d² (d in mm), from 7.76 g/cm³ density; lb/ft = kg/m × 0.672. Finished-part weights for your exact geometry are quoted on request.

Threads, Tolerances & Dimensional Standards

  • Inch threads: UNC, UNF and UN8 series per ASME B1.1 — the default for aerospace-style PH13-8Mo bolting.
  • Metric threads: standard M profile per ISO 261 / ISO 965 on request.
  • Rolled threads by default for fatigue performance; cut or ground threads supplied where geometry requires.
  • Dimensional standards: ANSI/ASME B18.2.1 (hex and heavy hex bolts), B18.2.2 (nuts), B18.3 (socket screws), with DIN, ISO, BS and GB equivalents — or your drawing.
  • Thread gauging: GO / NO-GO gauge inspection with results available in the inspection report.

How to Buy PH13-8Mo Fasteners from Calverbolt

What happens between your first email and the hardware arriving at your dock.

  1. RFQ & engineering review

    Send the drawing, standard or grade line. Our engineers confirm manufacturability and recommend the aging condition, thread class and finish for your service conditions.

  2. Quotation

    Pricing by lot size, certification level, finish and incoterm (EXW / FOB / CIF / DAP) — with the condition and test scope written into the offer.

  3. Sampling & first-article inspection

    Available before production release for new part numbers, with dimensional report against your drawing.

  4. Production & testing

    Melt-traceable bar, solution treatment, forming, aging to the ordered condition, mechanical testing, thread gauging and passivation — all certificate-backed.

  5. Packing & shipping

    Oiled and VCI-wrapped hardware in seaworthy crates, full export documentation, shipment to your port or door under the agreed incoterm.

Documentation checklist supplied with Calverbolt PH13-8Mo fastener orders
DocumentSupplied
EN 10204 type 3.1 material test certificateStandard with certified lots
Dimensional & thread-gauge inspection reportOn request / per drawing
PMI / OES chemistry verification recordOn request
NDT report (dye penetrant, eddy current)On request
Packing list, gross/net weightsStandard
Certificate of origin, export documentsStandard / per destination

PH13-8Mo Fasteners — Frequently Asked Questions

What is PH13-8Mo stainless steel?

PH13-8Mo (13-8 Mo, UNS S13800, EN/DIN 1.4534) is a martensitic precipitation-hardening (maraging) stainless steel that combines very high strength with superior toughness and good resistance to general corrosion and stress-corrosion cracking. Its nominal chemistry is 12.25–13.25% chromium, 7.50–8.50% nickel, 2.00–2.50% molybdenum and 0.90–1.35% aluminium, with carbon limited to 0.05% max. Tight composition control and vacuum melting give it excellent transverse toughness and minimal directionality.

Who manufactures PH13-8Mo / UNS S13800 fasteners in China?

Jiangsu Calverbolt Fasteners Co., Ltd., based in the Shiyan Town Alloy Industrial Park in Dongtai, Jiangsu Province, China, manufactures and exports PH13-8Mo (UNS S13800 / EN 1.4534) stainless steel fasteners — hex bolts, heavy hex bolts, stud bolts, threaded rod, socket head cap screws, nuts and washers — in diameters 1/4" to 4" and in aging conditions from H950 to H1150. Contact sales@calverbolt.com or WhatsApp +86 135 8506 7993 for a quote.

What is the EN / DIN equivalent of UNS S13800?

The European EN / DIN equivalent of UNS S13800 (PH13-8Mo) is material number 1.4534. Other designations for the same grade include PH 13-8 Mo stainless and 13-8Mo.

Which heat-treatment conditions do you supply?

Calverbolt supplies PH13-8Mo fasteners in Condition A (solution treated) and in the precipitation-hardened conditions H950, H1000, H1025, H1050, H1100, H1150, plus RH950 and H1150M. Aging is carried out at 950–1150 °F (510–621 °C) for 4 hours followed by air cooling. H1000 is the most common choice for airframe and structural bolting because it balances maximum strength, fracture toughness and stress-corrosion-cracking resistance.

PH13-8Mo vs 17-4PH (UNS S17400) — which should I specify?

PH13-8Mo and 17-4PH reach a similar strength class, but PH13-8Mo offers distinctly better transverse toughness, less directionality and superior stress-corrosion-cracking resistance, especially in marine atmospheres and in large sections. 17-4PH is more economical and more widely stocked, so engineers specify PH13-8Mo fasteners when the joint needs high strength plus high toughness under sustained load.

What specifications apply to your PH13-8Mo fasteners?

We manufacture PH13-8Mo fastener components from bar and forging stock to AMS 5629 and ASTM A564, with sheet, strip and plate to AMS 5864. Dimensions follow ANSI/ASME, ASTM, DIN, ISO, BS or GB standards or customer drawings. Every shipment can be supplied with an EN 10204 type 3.1 material test certificate showing chemistry and mechanical test results for the certified lot.

What sizes and product forms are available?

Diameters run from 1/4 inch to 4 inch, with metric equivalents on request. Product forms include hex bolts, heavy hex bolts, stud bolts and threaded rod, socket head cap screws, hex and heavy hex nuts, flat and lock washers, pins, and fully customised made-to-drawing parts produced by cold heading and machining.

How corrosion resistant is PH13-8Mo?

In the H950 condition, PH13-8Mo shows rusting resistance similar to Type 304 stainless steel in a 5% salt-fog test, and its general corrosion resistance approaches Type 304 in atmospheric and acid exposures. The alloy exhibits a high level of stress-corrosion-cracking resistance in marine atmospheric testing; for the best SCC resistance, specify an aging temperature of at least 1000 °F (538 °C) — conditions H1000 and above. Finished fasteners are passivated for optimum corrosion performance.

What are typical applications?

Typical uses are airframe structural components and landing-gear parts, valve parts and fittings, cold-headed and machined fasteners, shafts and pins, nuclear reactor components, petrochemical equipment requiring SCC resistance, and injection-molding equipment. Wherever a fastener needs high strength, high toughness and corrosion resistance with minimal property directionality, PH13-8Mo is the standard choice.

How do I get a quote?

Email sales@calverbolt.com or message WhatsApp +86 135 8506 7993 with the fastener type, standard or drawing, diameter and length, PH13-8Mo aging condition (e.g. H1000), finish and quantity. Jiangsu Calverbolt Fasteners Co., Ltd. replies with pricing, lead time and certification options — EN 10204 3.1 certificates included on request.

What does "13-8" mean in PH13-8Mo?

The name describes the nominal chemistry: roughly 13% chromium and 8% nickel, with molybdenum ("Mo") added for corrosion and temper resistance and aluminium as the aging element. The same convention names 17-4PH — 17% chromium, 4% nickel.

Is PH13-8Mo magnetic?

Yes. As a martensitic precipitation-hardening grade, PH13-8Mo is ferromagnetic in every condition, with relative permeability values in the order of 46–127 depending on field strength. Bolting can therefore be inspected by magnetic-particle methods — but it will attract a magnet and is not a non-magnetic substitute for 316.

What is Condition A?

Condition A is the solution-treated state: heated to 1675–1725 °F (910–940 °C), held about 15–30 minutes depending on section, then cooled below 60 °F (15 °C) so the structure transforms fully to martensite. Fastener forming and machining are normally done in Condition A, before final aging.

RH950 vs H950 — what is the difference?

Both age at 950 °F for 4 hours, but the RH950 route adds a subzero treatment at −100 °F for at least 2 hours, applied within 24 hours of solution treating, before aging. The cold treatment raises strength in heavier sections and appears in some airframe specifications; RH950 fasteners are quoted to order.

What is condition H1150M?

H1150M ages first at 1400 °F for 2 hours and then at 1150 °F for 4 hours. It is an overaged, maximum-toughness condition used mainly for machinability: parts are machined in H1150M, then re-solution treated and re-aged to the final specified condition.

What temperatures can PH13-8Mo fasteners serve at?

The alloy resists oxidation up to about 1100 °F (593 °C). For continuous service, avoid long exposure in the 600–900 °F (315–480 °C) band, where toughness can fall in PH grades — or specify a higher aging condition. Short excursions should stay at least 50 °F (28 °C) below the aging temperature.

Can PH13-8Mo be welded?

Yes, with care. Marine atmospheric test data on welded specimens show that welded-and-re-aged joints keep a high level of stress-corrosion-cracking resistance. Best practice: weld in the solution-treated condition, then re-solution treat and age. Brazing may be done in inert atmospheres; reducing atmospheres should be avoided because of the risk of nitrogen contamination.

Why should PH13-8Mo fasteners be passivated?

For optimum corrosion resistance the finished surface must be free of scale, heat tint and embedded iron. Pickling followed by passivation restores the passive chromium-oxide film after heat treatment and machining, and is part of Calverbolt's standard finishing for PH13-8Mo hardware.

Rolled or cut threads for high-strength bolts?

Rolled threads are preferred wherever the specification allows: the thread is formed rather than cut, so grain flow follows the thread profile and fatigue performance improves — an important advantage at 200-ksi-class strength. Calverbolt rolls PH13-8Mo threads by default and cuts or grinds only where geometry requires.

How heavy is PH13-8Mo, for shipping and costing?

Density is 7.76 g/cm³ (0.280 lb/in³) in the H1000 condition. The rod weight table above lists kg/m and lb/ft by diameter; finished-part weights for your exact geometry are quoted on request.

PH13-8Mo Terminology — Plain-Language Glossary

The words your drawing, test certificate and quote use, decoded.

Precipitation hardening
Strengthening by holding the metal at a moderate temperature so intermetallic precipitates — here aluminium-rich NiAl — form inside the martensitic matrix and block dislocation movement.
Maraging
Martensitic + aging: a low-carbon steel that hardens by aging rather than by carbon, giving high strength with unusually high toughness.
Condition A
The solution-treated state: held at 1675–1725 °F (910–940 °C), then cooled below 60 °F (15 °C) to fully transform to martensite. The soft, machinable starting point for forming and aging.
H950–H1150
Aged conditions: held at the stated temperature (°F) ±10 °F for 4 hours and air cooled. Lower numbers = stronger; higher numbers = tougher.
RH950
Aging route with a subzero step: −100 °F for at least 2 hours within 24 hours of solution treating, then aged at 950 °F. Raises strength in heavier sections.
H1150M
Double-aged, overaged condition: 1400 °F for 2 hours plus 1150 °F for 4 hours. Maximum toughness and machinability; parts are re-solution treated and re-aged to final properties.
Transverse toughness
Toughness measured across the bar direction rather than along it. PH13-8Mo's signature property: tight chemistry control and vacuum melting make properties nearly the same in every direction.
SCC
Stress-corrosion cracking — cracking under sustained tensile load in a corrosive environment. The reason specifiers move from 17-4PH to PH13-8Mo in marine and chemical atmospheres.
VIM / VAR
Vacuum induction melting and vacuum arc remelting — the melt routes that remove impurities and gases, producing the cleanliness behind the grade's transverse toughness.
Passivation
Acid treatment (nitric or citric) of finished stainless parts that removes free iron and rebuilds the protective chromium-oxide film.
ksi / MPa
Strength units: 1 ksi = 6.895 MPa. PH13-8Mo H950 minimum tensile strength, 220 ksi, equals about 1517 MPa.
EN 10204 3.1
A material test certificate issued by the manufacturer's inspection representative who is independent of the production department — the certification level most buyers require for PH13-8Mo bolting.

Technical References

Independent sources behind the data on this page.

  • Rolled Alloys, "Data Sheet 13-8 Stainless", Bulletin No. 1022 — chemistry, heat treatment, AMS 5864 minimum properties — rolledalloys.com (PDF)
  • High Temp Metals, "PH 13-8 Mo Technical Data" — type analysis, corrosion and stress-corrosion test data, fabrication practice — hightempmetals.com
  • Steel Service Associates, "13-8 PH Stainless – AMS 5629 – UNS S13800" — ssa-corp.com
  • 17-4PH comparison minimums, AMS 5643 — ssa-corp.com
  • 15-5PH comparison minimums, AMS 5659 — ssa-corp.com
  • A286 aged comparison minimums, AMS 5737 — aircraftmaterials.com
  • Inconel 718 comparison minimums, AMS 5662 — ssa-corp.com; Special Metals "INCONEL Alloy 718" bulletin — specialmetals.com (PDF)

Specifications are cited for education; the governing document for any order is the issue your purchase order specifies. INCONEL is a trademark of Special Metals Corporation.

Request a PH13-8Mo Fastener Quote

Send your standard, grade or drawing — a sales engineer replies with pricing, lead time and the certification options that fit your project.

Works Address

Jiangsu Calverbolt Fasteners Co., Ltd. · Shiyan Town Alloy Industrial Park, Dongtai, Jiangsu Province, China

Include in your RFQ

  • Fastener type and standard — or a drawing (PDF/STEP accepted)
  • Diameter and length, thread class (UNC/UNF or metric)
  • PH13-8Mo aging condition — e.g. H1000 — or the properties you need
  • Finish: pickled & passivated, or as-processed
  • Quantity, required delivery schedule and destination port
  • Certification: EN 10204 3.1, inspection reports, NDT scope